Table 3 Properties of fresh and hardened concrete.

From: Effect of Wet Curing Duration on Long-Term Performance of Concrete in Tidal Zone of Marine Environment

Code

Density (kg/m3)

Air content (%)

Slump (mm)

Curing

Compressive strength (MPa)

7 days

28 days

NPC

2370

2.7

80

0-D

26.0

31.3

1-D

30.0

36.6

3-D

30.8

37.9

6-D

33.5

39.0

27-D

33.5

39.8

SFC

2355

1.6

65

0-D

26.0

37.1

1-D

29.9

45.3

3-D

32.9

51.4

6-D

34.4

53.6

27-D

34.4

55.2