Skip to main content

Table 6 C30/37 strength class concrete mix design.

From: Temperature Reduction of Concrete Pavement Using Glass Bead Materials

Strength class C30/37

Cement PC 42.5 (kg)

Water (kg)

Glass bead (kg)

0/4 Fine aggregate (kg)

7/15 Coarse aggregate (kg)

15/25 Coarse aggregate (kg)

Admixture (g)

0 % Glass bead

1.50

0.87

0

4.874

2.343

2.164

18

9 % Glass bead

1.50

0.87

0.798

3.562

2.343

2.164

18

19 % Glass bead

1.50

0.87

1.597

2.25

2.343

2.164

18

31 % Glass bead

1.50

0.87

2.395

0.937

2.343

2.164

18