Skip to main content

Table 2 Mixture design for HRPC and PRPC.

From: Effects of Temperature and Stress on Creep Behavior of PP and Hybrid Fiber Reinforced Reactive Powder Concrete

Constituents

HPRPC

PRPC

Ordinary Portland cement (kg/m3)

815.18

816.42

Silica fume (kg/m3)

245.31

244.33

Slag (kg/m3)

120.08

122.16

Quartz coarse sand (kg/m3)

480.32

490.32

Quartz fine sand (kg/m3)

480.32

490.32

Water reducer (kg/m3)

35.40

35.47

PP fiber (kg/m3)

1.82 (0.2%a)

2.73 (0.3%a)

Steel fiber (kg/m3)

157 (2%a)

–

Water (kg/m3)

188.81

189.20

w/b ratio

0.16

0.16

  1. aSteel and PP fibers are measured as % of RPC volume.