Table 5 Air content and slump measurement results.

From: Mechanical Behavior of Recycled Fine Aggregate Concrete with High Slump Property in Normal- and High-Strength

Specimen ID

Air content (%)

Slump (mm)

Measured

Avg. (COV)

Measured

Avg. (COV)

NS concrete

 30-R0

5.2

5.3 ± 0.21 (4.0%)

210

214 ± 5.5 (2.6%)

 30-R15

5.6

220

 30-R30

5.0

220

 30-R50

5.3

215

 30-R100

5.5

205

HS concrete

 60-R0

3.7

3.3 ± 0.24 (7.2%)

220

217 ± 2.4 (1.1%)

 60-R15

3.3

215

 60-R30

3.0

215

 60-R50

3.5

220

 60-R100

3.2

215