Name | Fiber incorporated | Vf (%) | Fiber (kg/m3) | C (kg/m3) | CA (kg/m3) | FA (kg/m3) | W (kg/m3) | w/c |
---|---|---|---|---|---|---|---|---|
Mix ID—1 | None | 0.00 | 0.0 | 503.3 | 709.7 | 986.5 | 201.3 | 0.40 |
Mix ID—2 | Polypropylene | 0.50 | 4.5 | 500.8 | 706.1 | 981.5 | 200.3 | 0.40 |
Mix ID—3 | 0.75 | 6.8 | 499.5 | 704.3 | 979.1 | 199.8 | 0.40 | |
Mix ID—4 | 1.00 | 9.1 | 498.3 | 702.6 | 976.6 | 199.3 | 0.40 | |
Mix ID—5 | 0.75 | 6.8 | 487.3 | 687.1 | 955.0 | 219.3 | 0.45 | |
Mix ID—6 | 0.75 | 6.8 | 475.6 | 670.6 | 932.1 | 237.8 | 0.50 | |
Mix ID—7 | Nylon | 0.50 | 5.7 | 500.8 | 706.1 | 981.5 | 200.3 | 0.40 |
Mix ID—8 | 0.75 | 8.5 | 499.5 | 704.3 | 979.1 | 199.8 | 0.40 | |
Mix ID—9 | 1.00 | 11.4 | 498.3 | 702.6 | 976.6 | 199.3 | 0.40 | |
Mix ID—10 | 0.75 | 8.5 | 487.3 | 687.1 | 955.0 | 219.3 | 0.45 | |
Mix ID—11 | 0.75 | 8.5 | 475.6 | 670.6 | 932.1 | 237.8 | 0.50 | |
Mix ID—12 | Glass | 0.50 | 13.5 | 500.8 | 706.1 | 981.5 | 200.3 | 0.40 |
Mix ID—13 | 0.75 | 20.2 | 499.5 | 704.3 | 979.1 | 199.8 | 0.40 | |
Mix ID—14 | 1.00 | 27.0 | 498.3 | 702.6 | 976.6 | 199.3 | 0.40 | |
Mix ID—15 | 0.75 | 20.2 | 487.3 | 687.1 | 955.0 | 219.3 | 0.45 | |
Mix ID—16 | 0.75 | 20.2 | 475.6 | 670.6 | 932.1 | 237.8 | 0.50 | |
Mix ID—17 | Steel | 0.50 | 39.0 | 500.8 | 706.1 | 981.5 | 200.3 | 0.40 |
Mix ID—18 | 0.75 | 58.5 | 499.5 | 704.3 | 979.1 | 199.8 | 0.40 | |
Mix ID—19 | 1.00 | 78.0 | 498.3 | 702.6 | 976.6 | 199.3 | 0.40 | |
Mix ID—20 | 0.75 | 58.5 | 487.3 | 687.1 | 955.0 | 219.3 | 0.45 | |
Mix ID—21 | 0.75 | 58.5 | 475.6 | 670.6 | 932.1 | 237.8 | 0.50 |