Skip to main content

Table 2 Average peak compressive strength and compressive toughness index (CTI).

From: A Study on Residual Compression Behavior of Structural Fiber Reinforced Concrete Exposed to Moderate Temperature Using Digital Image Correlation

Fiber dosage (kg/m3)

Property

Room temperature

150 °C

200 °C

300 °C

0

Strength (MPa)

55.2 (0.7)

54.2 (1.2)

48.6 (2.4)

42.3 (1.4)

CTI (×10−3)

5.3 (0. 08)

4.3 (0. 05)

4.1 (0. 1)

4.3 (0. 05)

4

Strength (MPa)

55.7 (1.8)

53.3 (1.6)

52.4 (0.7)

48.7 (2.1)

CTI (×10−3)

10.3 (0. 06)

8.4 (0. 05)

7.6 (0. 04)

6.8 (0. 04)

5

Strength (MPa)

56.8 (1.4)

55.1 (1.8)

54.3 (1.2)

50.4 (2.3)

CTI (×10−3)

14.2 (0. 03)

10.2 (0. 09)

9.4 (0. 07)

8.7 (0. 06)

6

Strength (MPa)

57.5 (0.9)

56.2 (2.2)

55.4 (2.1)

51.3 (3.1)

CTI(×10−3)

18.3 (0. 02)

14.2 (0. 06)

11.8 (0. 08)

9.4 (0. 09)

  1. The values in the parenthesis indicate standard deviation.