From: Effect of Fiber Hybridization on Durability Related Properties of Ultra-High Performance Concrete
Property of UHPC | C1 | SC | SPC1 | SPC2 | SPC3 | PC | C2 |
---|---|---|---|---|---|---|---|
Apparent density (g/cm3) | 2.57 | 2.61 | 2.51 | 2.45 | 2.36 | 2.30 | 2.40 |
Absorptivity (%) | 0.60 | 0.54 | 0.69 | 0.78 | 0.95 | 1.07 | 0.75 |
Compressive strength (MPa) | 151.0 | 154.9 | 144.7 | 133.9 | 122.3 | 94.6 | 129.5 |
Splitting tensile strength (MPa) | 8.9 | 13.8 | 13.5 | 10.0 | 9.3 | 7.6 | 6.8 |
Modulus of elasticity (GPa) | 38.37 | 39.74 | 34.27 | 32.45 | 29.60 | 29.42 | 32.55 |