Table 5 Dynamic compressive performances of various samples.

From: Dynamic Properties of Strain-Hardening Cementitious Composite Reinforced with Basalt and Steel Fibers

Specimen ID

Strain rate (s−1)

Compressive strength (MPa)

Failure strain (× 10−6)

BF0SF0

36.1

36.8

6530

55.4

43.0

5693

77.7

46.6

6043

202.3

58.4

7253

BF3SF0

44.2

39.1

8550

66.2

47.5

8047

76.9

53

5320

172.8

60.7

5967

BF2.5SF0.5

43.2

39.2

7950

51.8

40.1

6250

80.8

56.0

7060

190.8

61.9

6910

BF2SF1

40.4

41.1

6490

53.1

42.3

5370

84.0

57.1

6290

182.9

63.0

7230