From: Influence of Fe2O3 Nanoparticles on the Characteristics of Waste Marble Powder Mixed Cement Mortars
Sample ID | W/B | Flow Spread (mm) | Compressive strength-28th day (MPa) | Split Tensile strength-28th day (MPa) |
---|---|---|---|---|
C-1 | 0.5 | 283 | 33.38 | 2.46 |
MP-5 | 0.5 | 289 | 34.65 | 2.51 |
MP-10 | 0.5 | 292 | 35.54 | 2.59 |
MP-15 | 0.5 | 286 | 32.74 | 2.36 |
MP-20 | 0.5 | 273 | 29.72 | 2.04 |
NF-1 | 0.5 | 292 | 35.28 | 3.19 |
NF-2 | 0.5 | 297 | 37.54 | 3.27 |
NF-3 | 0.5 | 282 | 29.42 | 1.94 |
NF-4 | 0.5 | 271 | 24.68 | 1.52 |