Skip to main content

Table 5 Mix proportion for wet packing density test with recycled sand

From: Mechanical Properties of Ultra-High Performance Concrete (UHPC) and Ultra-High Performance Fiber-Reinforced Concrete (UHPFRC) with Recycled Sand

Index

Volume-base (m3)

OPC

FA

SF

QP

RS

W

Total

W-RS-1

0.260

0.029

0.072

0.000

0.442

0.196

1.0

W-RS-2

0.260

0.029

0.054

0.018

0.441

0.197

1.0

W-RS-3

0.260

0.029

0.036

0.036

0.441

0.199

1.0

W-RS-4

0.259

0.029

0.018

0.054

0.440

0.200

1.0

Index

Mass-base (kg/m3)

OPC

FA

SF

QP

RS

W

Theoretical wt

W-RS-1

820

72

161

0

1088

196

2337

W-RS-2

819

72

120

48

1086

197

2343

W-RS-3

818

72

80

96

1084

199

2348

W-RS-4

817

72

40

143

1082

200

2354

  1. 1. W-RS-n, W wet packing, RS recycled sand, n batch number; 2. binder:sand = 45%:55% by vol.; 3. FA replaces OPC by 10% by vol.; 4. (SF + QP) replaces binder by 20% by vol.; 5. SF:QP = 20%:0%, 15%:5%, 10%:10%, 5%:15%; 6. W/B = 0.20; 7. SP and DF amount is 4.0% and 0.1% of total binder amount, respectively, in all mixes